Testing of materials
Standard lab methods to determine strength, ductility, stiffness, hardness, impact energy, and time-dependent behavior of materials using tensile, hardness, impact, torsion, fatigue, and creep tests, and how to interpret the results.
Drafted with Aria, reviewed by the AiCanCode.org team · Updated . How we write and check our notes. Spotted an error? Use Give Feedback at the bottom of the page.
Why it matters
Testing tells you what a real material can actually take before it yields, breaks, dents, or fails over time. Designers turn test results into allowable stresses and safety margins for shafts, beams, pressure parts, and fasteners.
Key ideas
- Test specimen: A standardized piece cut or machined from a material to ensure repeatable geometry, surface finish, and gauge length so different labs and engineers can compare results meaningfully.
- Engineering (nominal) stress, σ: Load divided by the original cross-sectional area,
σ = P / A0. It assumes area stays constant; this is convenient for plotting and for design comparisons. - Engineering (nominal) strain, ε: Change in gauge length divided by the original gauge length,
ε = ΔL / L0. - True stress, σ_true: Instantaneous load divided by the current (instantaneous) area,
σ_true = P / Ai. It captures the fact that the specimen necks and area shrinks in plasticity. - True (logarithmic) strain, ε_true:
ε_true = ln(L / L0). For uniform deformation (before necking and assuming approximately constant volume),σ_true = σ (1 + ε)andε_true = ln(1 + ε). - Stress–strain curve (tension): For a ductile metal (e.g., mild steel) the curve typically has: linear elastic region (slope = E), proportional limit, yield point (sometimes upper/lower yield), plastic hardening up to ultimate tensile strength (UTS), then necking to fracture. For many ductile metals, maximum engineering load (UTS) coincides with the onset of necking (Considère criterion), which satisfies
dσ_true/dε_true = σ_true. - Elastic modulus, E: Slope of the initial linear part of the stress–strain curve; describes stiffness. Determined from precise extension measurements (extensometer).
- Yield strength: For materials without a clear yield point, the 0.2% proof stress is used: draw a line parallel to the elastic slope offset by ε = 0.002 and find its intersection with the curve. For mild steel with Lüders bands you may observe upper and lower yield points.
- Ultimate tensile strength (UTS): Maximum engineering stress
σu = Pmax / A0. - Ductility measures: Percentage elongation
(Lf − L0)/L0 × 100%and percentage reduction of area(A0 − Af)/A0 × 100%measured after fracture over the gauge length. - Resilience and toughness: Resilience is elastic energy per unit volume up to yield (area under elastic part); modulus of resilience
Ur = σy²/(2E)for linear-elastic up to σy. Toughness is total energy per unit volume to fracture (total area under the stress–strain curve). - Test machines and control: Universal testing machine (UTM) applies axial load under controlled crosshead speed, stress rate, or strain rate. Use an extensometer in the gauge length for accurate elastic data. Machine compliance and misalignment must be minimized or corrected.
- Standard specimens and gauge length: For metallic tension testing at room temperature, proportional specimens often use
L0 = 5.65 √A0so that elongation results are comparable across sizes (from ISO-harmonized standards used in India). Non-proportional (fixed-length) specimens are also used; always report the gauge length. - Compression test: Useful for brittle materials or plastics; avoid slenderness that would cause buckling. Friction at platens induces barreling; lubricate or use suitable platens to reduce it.
- Hardness: Resistance to permanent indentation. Common tests:
- Brinell (HBW): 10 mm hard ball indenter, heavy load; measures indentation diameter; good for coarse-grained or heterogeneous metals.
- Vickers (HV): Diamond pyramid (136°) indenter; measures diagonal length; one scale suitable for wide hardness range; useful on thin sections.
- Rockwell (HR): Depth-based measurement with minor + major load; multiple scales (A, B, C, etc.) for different materials; quick, no optical reading.
- Impact tests: Charpy V-notch and Izod measure energy absorbed in fracturing a notched specimen by a swinging pendulum. Report absorbed energy and note temperature sensitivity (ductile-to-brittle transition in many BCC steels).
- Torsion test: For circular shafts, measures torque-angle response; in the elastic range, slope gives shear modulus G; beyond elastic, torsional yield and plasticity can be studied. Use
τ = Tc/Jandθ = TL/(JG)in the elastic range. - Fatigue testing (S–N test): Repeated cyclic loading (e.g., rotating-bending) at constant stress amplitude to get cycles-to-failure N. The S–N curve shows stress amplitude versus log N; ferrous alloys may show an endurance limit.
- Creep test: Constant stress at elevated temperature; measure strain versus time. Creep curve has primary (decelerating), secondary (steady-rate), and tertiary (accelerating) stages; time to rupture is a key result.
- Assumptions and realities:
- Stress and strain are uniform in the gauge length until necking; after necking, true stress requires local area measurement.
- Extensometer readings reflect material strain; crosshead travel includes machine compliance.
- Surface finish, temperature, and strain rate affect measured yield, UTS, ductility, and impact energy. Standards prescribe control of these factors.
- Sign convention: Tension positive, compression negative for normal stress; report shear stress magnitude and direction separately.
Formulas
σ = P / A0 — Engineering stress; P: axial load (N), A0: original area (mm²). Gives σ in N/mm² = MPa. Valid for nominal stress in tension/compression.
ε = ΔL / L0 — Engineering strain; ΔL: extension (mm), L0: original gauge length (mm). Dimensionless. Valid for small and large strains as nominal measure.
σ_true = P / Ai — True stress; P: load (N), Ai: instantaneous area (mm²). Gives MPa. Valid at any stage; requires current area.
σ_true = σ (1 + ε) — Relation between true and engineering stress during uniform deformation (before necking), assuming approximately constant volume. σ, ε as above. MPa for stress, dimensionless strain.
ε_true = ln(1 + ε) — True (logarithmic) strain from engineering strain during uniform deformation.
E = (σ / ε) — Young’s modulus (elastic slope); E in MPa when σ in MPa, ε dimensionless. Valid in initial linear-elastic range.
Ur = σy² / (2E) — Modulus of resilience; σy: yield strength (MPa), E: Young’s modulus (MPa). Ur in MPa (numerically equal to MJ/m³). Valid for linear-elastic behavior up to yield.
% elongation = (Lf − L0) / L0 × 100% — Ductility measure after fracture; lengths in mm.
% reduction of area = (A0 − Af) / A0 × 100% — Ductility measure after fracture; areas in mm².
HBW (MPa) = 2F / [π D (D − √(D² − d²))] — Brinell hardness as mean contact pressure; F: force (N), D: ball diameter (mm), d: indentation diameter (mm). Result in MPa. Traditional BHN in kgf/mm² = HBW(MPa)/9.80665. Applicable for valid Brinell test conditions.
HV (MPa) ≈ 1.854 F / d² — Vickers hardness; F: force (N), d: average diagonal of indentation (mm). Result approximates MPa when using SI; valid for standard 136° diamond pyramid.
HR = N − (h − h0)/S — Rockwell number; h−h0: permanent depth increase (mm), S = 0.002 mm per Rockwell unit, N depends on scale (e.g., N = 100 for HRC, N = 130 for HRB). Loads and indenters per chosen scale. Dimensionless.
U = m g (h1 − h2) — Charpy/Izod absorbed energy from pendulum; m: mass (kg), g: 9.81 m/s², h1, h2: vertical heights (m). U in J. Valid if friction/windage corrections negligible or accounted for.
τ = T c / J — Shear stress in circular shaft under torque; T: torque (N·m), c: radius (m), J: polar second moment (m⁴). Valid in elastic range and Saint-Venant theory.
θ = T L / (J G) — Angle of twist; θ: radians, L: gauge length (m), G: shear modulus (Pa). Valid in elastic range for prismatic, homogeneous shafts.
Jsolid = π d⁴ / 32 — Polar second moment for solid circular shaft; d in m (or mm with consistent units).
Jhollow = π (Do⁴ − Di⁴) / 32 — Polar second moment for hollow circular section; diameters consistent.
S N^b = C — Basquin’s law for high-cycle fatigue; S: stress amplitude (MPa), N: cycles to failure, b, C: material constants from S–N data. Empirical, log–log linear region.
ε̇s = Δε / Δt — Steady-state creep rate; ε̇s in s⁻¹; ε dimensionless, t in s. Applicable to secondary creep.
UTS (MPa) ≈ 3.45 × HB (BHN) — Empirical for steels: UTS in MPa from Brinell hardness number BHN (kgf/mm²). Rough estimate only.
Worked examples
Example 1 (direct): Brinell hardness and UTS estimate Given: steel specimen tested with Brinell 10 mm ball at F = 29.4 kN, measured indentation diameter d = 4.00 mm. Estimate HBW (MPa), BHN, and UTS.
- Brinell hardness (MPa)
- Formula:
HBW = 2F / [π D (D − √(D² − d²))] - Numbers: D = 10.00 mm, F = 29,400 N, d = 4.00 mm
- Compute √(D² − d²) = √(100 − 16) = √84 = 9.165 mm
- D − √(...) = 10.000 − 9.165 = 0.835 mm
- Denominator = π × 10 × 0.835 ≈ 26.223 mm²
- Numerator = 2F = 58,800 N
- HBW = 58,800 / 26.223 ≈ 2,243.5 N/mm² = 2,243.5 MPa
- Answer: HBW ≈ 2,244 MPa
- Convert to BHN (traditional units)
BHN = HBW / 9.80665 = 2,243.5 / 9.80665 = 228.7- Answer: BHN ≈ 229
- Estimate UTS (empirical, steels)
UTS ≈ 3.45 × BHN = 3.45 × 228.7 = 789.8 MPa- Final: UTS ≈ 790 MPa (approximate)
Example 2 (GATE-level): Tension test data interpretation with true quantities and ductility A machined steel tensile specimen has original diameter d0 = 10.0 mm and gauge length L0 = 50.0 mm. In the elastic region, at P = 15.0 kN the measured extension is ΔL = 0.050 mm (using an extensometer). Yield load is Py = 28.0 kN, maximum load is Pmax = 42.0 kN. The total extension at Pmax is measured as ΔLu = 2.40 mm. After fracture, the gauge length is Lf = 59.0 mm and the minimum (neck) diameter at the fracture is df = 6.80 mm. Determine: (a) E, (b) σy and σu (engineering), (c) percentage elongation and percentage reduction of area, (d) true stress and true strain at the maximum load (assume uniform deformation up to UTS).
Given data:
- d0 = 10.0 mm ⇒
A0 = π d0² / 4 = π × 10² / 4 = 78.540 mm² - L0 = 50.0 mm
- P (elastic point) = 15.0 kN = 15,000 N; ΔL = 0.050 mm
- Py = 28.0 kN; Pmax = 42.0 kN
- ΔLu = 2.40 mm at Pmax
- Lf = 59.0 mm; df = 6.80 mm ⇒
Af = π df² / 4 = π × 6.80² / 4 = 36.317 mm²
Steps:
- Elastic modulus E
- Formula:
E = (P L0) / (A0 ΔL) - Numbers: E = (15,000 N × 50.0 mm) / (78.540 mm² × 0.050 mm)
- Compute denominator: 78.540 × 0.050 = 3.927 mm³
- Numerator: 750,000 N·mm
- E = 750,000 / 3.927 = 190,987 N/mm² = 190,987 MPa
- Answer: E ≈ 191 GPa
- Engineering yield strength and UTS
σy = Py / A0 = 28,000 / 78.540 = 356.6 MPaσu = Pmax / A0 = 42,000 / 78.540 = 534.8 MPa- Answers: σy ≈ 357 MPa, σu ≈ 535 MPa
- Ductility measures
- Percentage elongation:
((Lf − L0)/L0) × 100% = (59.0 − 50.0)/50.0 × 100% = 18.0% - Percentage reduction of area:
((A0 − Af)/A0) × 100% = (78.540 − 36.317)/78.540 × 100% = 53.8% - Answers: % elongation = 18.0%, %RA = 53.8%
- True stress and true strain at the maximum load (assume uniform deformation up to UTS)
- Engineering strain at maximum load:
εu = ΔLu / L0 = 2.40 / 50.0 = 0.0480 - True strain:
ε_true,u = ln(1 + εu) = ln(1.0480) = 0.0469 - True stress:
σ_true,u = σu × (1 + εu) = 534.8 × 1.0480 = 560.5 MPa - Answers: ε_true,u ≈ 0.0469, σ_true,u ≈ 560 MPa
Assumptions: axial load concentric, uniform deformation holds up to UTS, extensometer spans exactly L0, temperature ~ room temperature.
Common mistakes
- Reading extension from crosshead travel instead of an extensometer in the elastic range (machine compliance causes error in E and proof stress).
- Mixing units (N with mm², kgf with N) in hardness or stress calculations.
- Confusing yield strength with 0.2% proof stress, or forgetting to draw the offset line parallel to the elastic slope.
- Reporting percentage elongation without stating the gauge length standard (proportional vs fixed).
- Using hardness-to-UTS empirical conversion outside its valid material family (e.g., applying steel correlation to aluminum).
- Rockwell scale misuse: wrong indenter or load for the material thickness; reading HRC for soft metals or HRB for hardened steels.
- Ignoring strain rate and temperature in impact testing; transition temperature effects can dominate Charpy energy for BCC steels.
For GATE ME
- Conceptual questions on differences between engineering vs true stress/strain, why UTS corresponds to necking in ductile metals, and interpretation of stress–strain curves (yielding, strain hardening, ductility metrics).
- Numericals on: computing E from load–extension; computing σy, σu, % elongation, %RA; estimating modulus of resilience; converting between engineering and true quantities in the uniform region.
- Hardness test calculations (Brinell, Vickers): compute HB/HV from indent dimensions and load; select appropriate hardness test for thin sections vs coarse microstructures; basic Rockwell scale facts.
- Impact test energy from pendulum heights; qualitative effects of temperature and notch.
- Torsion test in the elastic range to determine G using θ–T–L relation (the plastic torsion analysis belongs to Torsion of Circular Shafts topic).
- Fatigue and creep: identification of S–N curve features and creep curve stages in the context of “testing” (detailed life models are in Fatigue and Fracture Mechanics and Creep and Viscoelasticity).
- Practise: clean unit handling; careful reading of gauge lengths and diameters; drawing 0.2% offset line; carrying significant figures and uncertainty where needed.
Quick check
- In a tensile test, why is 0.2% proof stress used for some metals?
- Write the relation between true and engineering strain in the uniform deformation region.
- Which hardness test is best suited for thin, surface-hardened layers, and why?
Answers: 1) Because many metals (e.g., Al alloys) do not show a clear yield point; the 0.2% offset defines a reproducible yield criterion. 2) ε_true = ln(1 + ε). 3) Vickers (or Rockwell superficial) because the small diamond indenter and lower loads allow shallow impressions with minimal substrate influence.
Finished this topic? Mark it so your progress, study plan and readiness keep up.
Stuck on something here?