Engineering Materials

Engineering Materials — formula sheet

Production & Industrial Engineering · GATE PI · SI units. Drafted with Aria, checked by the AiCanCode.org team.

Crystal Structures and Miller Indices

  • n = Nc/8 + Nf/2 + Ni — atoms per cubic unit cell; Nc, Nf, Ni = corner, face and interior atoms. SC 1, BCC 2, FCC 4.
  • a = 2r (SC); a = 4r/√3 (BCC); a = 2√2·r (FCC) — lattice parameter a and atomic radius r (m).
  • APF = n·(4/3)π·r³ / a³ — atomic packing factor (dimensionless): SC 0.52, BCC 0.68, FCC and ideal HCP 0.74.
  • ρ = n·A / (NA·a³) — theoretical density (g/cm³ with a in cm); A = atomic mass (g/mol); NA = 6.022 × 10²³ mol⁻¹.
  • d_hkl = a / √(h² + k² + l²) — interplanar spacing of (hkl) planes (m); cubic crystals only.
  • n_r·λ = 2·d·sin θ — Bragg's law; n_r = order of reflection, λ = X-ray wavelength (m), θ = Bragg angle (half of 2θ).

Crystal Defects and Plastic Deformation

  • τR = σ·cos φ·cos λ — Schmid's law; τR = resolved shear stress (Pa), σ = applied uniaxial stress (Pa), φ = angle between load axis and slip-plane normal, λ = angle between load axis and slip direction. Maximum Schmid factor 0.5.
  • σy = τCRSS / (cos φ·cos λ) — single-crystal yield stress; τCRSS = critical resolved shear stress (Pa).
  • σy = σ0 + ky·d^(−1/2) — Hall–Petch; σ0 = friction stress (Pa), ky = locking parameter (Pa·m^½, from data), d = grain diameter (m).
  • Nv / N = exp(−Qv / (k·T)) — equilibrium vacancy fraction; Qv = formation energy (eV), k = 8.617 × 10⁻⁵ eV/K, T in K.
  • %CW = (A0 − Ad) / A0 × 100 — percent cold work; A0, Ad = original and deformed cross-sectional areas.

Stress-Strain Behaviour and Mechanical Properties

  • σ = F / A0 — engineering stress (Pa); F = load (N), A0 = original area (m²).
  • ε = ΔL / L0 — engineering strain (dimensionless); ΔL = elongation, L0 = original gauge length (m).
  • σ = E·ε — Hooke's law; E = Young's modulus (Pa); linear elastic region only.
  • ν = −ε_lateral / ε_axial and G = E / (2(1 + ν)) — Poisson's ratio; shear modulus G (Pa) for isotropic materials.
  • %EL = (Lf − L0)/L0 × 100 and %RA = (A0 − Af)/A0 × 100 — ductility; Lf, Af = gauge length and minimum area after fracture.
  • Ur = σy² / (2E) — modulus of resilience (J/m³); σy = yield strength (Pa).
  • σT = σ·(1 + ε) and εT = ln(1 + ε) — true stress (Pa) and true strain; valid up to the onset of necking.
  • σT = K·εTⁿ — Hollomon law; K = strength coefficient (Pa), n = strain-hardening exponent; necking starts at εT = n.

Hardness, Impact, Fatigue and Creep Testing

  • HB = 2F / (π·D·(D − √(D² − d²))) — Brinell hardness; F = load (kgf), D = ball diameter (mm), d = indentation diameter (mm). With F in N multiply by 0.102.
  • HV = 1.8544·F / d² — Vickers hardness; F = load (kgf), d = mean indentation diagonal (mm).
  • E_abs = m·g·(h1 − h2) — Charpy/Izod energy absorbed (J); m = hammer mass (kg), h1, h2 = heights before release and after the swing (m).
  • σm = (σmax + σmin)/2; σa = (σmax − σmin)/2; R = σmin/σmax — mean stress, stress amplitude (Pa) and stress ratio.
  • σa/Se + σm/Su = 1 — Goodman line; Se = endurance limit, Su = ultimate tensile strength (Pa).
  • σa = σf′·(2Nf)^b — Basquin's law; σf′ = fatigue strength coefficient (Pa), b = fatigue strength exponent, Nf = cycles to failure (constants from data).
  • ε̇s = A·σⁿ·exp(−Qc / (R·T)) — steady-state creep rate (s⁻¹); A, n from data; Qc = activation energy (J/mol); R = 8.314 J/(mol·K); T in K.
  • LMP = T·(C + log10 tr) — Larson–Miller parameter; T in K, tr = rupture time (h), C ≈ 20 for steels.

Phase Diagrams and the Lever Rule

  • F = C − P + 1 — Gibbs phase rule at constant pressure; F = degrees of freedom, C = components, P = phases in equilibrium.
  • Wα = (Cβ − C0) / (Cβ − Cα) and Wβ = (C0 − Cα) / (Cβ − Cα) — lever rule; C0 = alloy composition, Cα, Cβ = phase compositions at the ends of the tie line (same wt % units); W = weight fractions, Wα + Wβ = 1. Two-phase fields only.
  • Vα = (Wα/ρα) / (Wα/ρα + Wβ/ρβ) — weight fraction to volume fraction; ρ = phase densities.

Iron-Carbon Equilibrium Diagram

  • Key points — ferrite max 0.022 % C at 727 °C; austenite max 2.14 % C at 1147 °C; eutectoid 0.76 % C, 727 °C (γ → α + Fe₃C); eutectic 4.3 % C, 1147 °C (L → γ + Fe₃C); peritectic about 0.17 % C, 1493 °C (L + δ → γ); cementite 6.7 % C.
  • W_pearlite = (C0 − 0.022) / (0.76 − 0.022) and W_α,pro = (0.76 − C0) / (0.76 − 0.022) — hypoeutectoid steels, just below 727 °C; C0 in wt % C.
  • W_pearlite = (6.7 − C0) / (6.7 − 0.76) and W_Fe₃C,pro = (C0 − 0.76) / (6.7 − 0.76) — hypereutectoid steels, just below 727 °C.
  • W_α,total = (6.7 − C0) / (6.7 − 0.022) and W_Fe₃C,total = (C0 − 0.022) / (6.7 − 0.022) — total phase fractions below 727 °C.

TTT and CCT Diagrams

  • y = 1 − exp(−k·tⁿ) — Avrami equation; y = fraction transformed, t = time (s), k = rate constant (s⁻ⁿ), n = Avrami exponent (from data).
  • t_y = [−ln(1 − y) / k]^(1/n) and t₀.₅ = (ln 2 / k)^(1/n) — time to fraction y and half-transformation time (s).
  • CR_crit ≈ (T_γ − T_nose) / t_nose — rough critical cooling rate (°C/s); T_γ = austenitising temperature, T_nose and t_nose = nose temperature (°C) and time (s).

Heat Treatment: Annealing, Normalising, Hardening, Tempering

  • T ≈ A3 + (30 to 50) °C — full annealing and hardening of hypoeutectoid steels; hypereutectoid steels are hardened from A1 + (30 to 50) °C.
  • T ≈ A3 (or Acm) + (40 to 60) °C — normalising, then air cooling.
  • A3 ≈ 910 − 203·√C — empirical A3 (°C) of a plain carbon steel; C in wt %.
  • P = T·(C_HJ + log10 t) — Hollomon–Jaffe tempering parameter; T in K, t in h, C_HJ ≈ 20; equal P gives equal tempered hardness.

Surface Hardening: Carburising, Nitriding, Induction Hardening

  • (Cx − C0) / (Cs − C0) = 1 − erf( x / (2·√(D·t)) ) — Fick's second law, constant surface concentration; Cx = concentration at depth x (m), C0 = initial, Cs = surface (wt %), D = diffusivity (m²/s), t = time (s).
  • x ≈ √(D·t) and x1²/t1 = x2²/t2 — order-of-magnitude case depth; depth ∝ √t at fixed temperature.
  • D = D0·exp(−Q / (R·T)) — diffusivity (m²/s); D0, Q (J/mol) from data; T in K.
  • δ = 503·√(ρ / (μr·f)) — induction skin depth (m); ρ = resistivity (Ω·m), μr = relative permeability (1 above 768 °C), f = frequency (Hz).

Plain Carbon Steels, Alloy Steels and Cast Irons

  • CE = C + (Si + P)/3 — carbon equivalent of cast iron (wt %); below 4.3 hypoeutectic, above 4.3 hypereutectic.
  • CE_IIW = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15 — weldability carbon equivalent of steel (wt %); above about 0.45 preheating is normally needed (check the welding code).

Non-Ferrous Alloys: Aluminium, Copper and Titanium

  • Specific strength = σy / ρ and Specific stiffness = E / ρ — σy, E in Pa; ρ in kg/m³; result in J/kg.
  • R = ρe·L / A — electrical resistance (Ω); ρe = resistivity (Ω·m), L = length (m), A = area (m²).

Polymers: Structure and Properties

  • DP = Mn / m — degree of polymerisation; Mn = number-average molecular weight (g/mol), m = repeat-unit molar mass (g/mol).
  • Mn = Σ xi·Mi and Mw = Σ wi·Mi — number- and weight-average molecular weights; xi = number fraction, wi = weight fraction, Mi = mean molar mass of class i.
  • PDI = Mw / Mn — polydispersity index (≥ 1).
  • % crystallinity = ρc·(ρs − ρa) / [ρs·(ρc − ρa)] × 100 — ρs = sample density, ρc = fully crystalline density, ρa = fully amorphous density.

Ceramics and Their Properties

  • K = Y·σ·√(π·a) — stress-intensity factor (MPa·√m); fracture when K = KIC. Y = geometry factor, σ = tensile stress (MPa), a = surface-crack depth or half-length of an internal crack (m).
  • σf = KIC / (Y·√(π·a)) and a_c = (1/π)·(KIC / (Y·σ))² — fracture stress and critical flaw size.
  • Pf = 1 − exp[−(σ/σ0)^m] — Weibull failure probability; σ0 = characteristic strength, m = Weibull modulus.
  • ΔTc = σf·(1 − ν) / (E·α) — critical thermal-shock temperature jump (K); α = thermal expansion coefficient (K⁻¹).

Composite Materials

  • Ec,l = Ef·Vf + Em·Vm — longitudinal modulus of aligned continuous-fibre composite (isostrain); V = volume fractions.
  • 1/Ec,t = Vf/Ef + Vm/Em — transverse modulus (isostress).
  • Ff / Fm = Ef·Vf / (Em·Vm) — load ratio, fibres to matrix, under longitudinal loading.
  • σc,l = σf*·Vf + σm′·(1 − Vf) — longitudinal strength; σf* = fibre strength, σm′ = matrix stress at fibre failure.
  • lc = σf*·d / (2·τc) — critical fibre length (m); d = fibre diameter, τc = interfacial shear strength (Pa).
  • ρc = ρf·Vf + ρm·Vm — composite density.

Non-Destructive Testing Methods

  • λ = v / f — ultrasonic wavelength (m); v = sound velocity (m/s), f = frequency (Hz).
  • d = v·t / 2 — reflector depth in pulse-echo UT (m); t = round-trip time (s).
  • Z = ρ·v and R = [(Z2 − Z1)/(Z2 + Z1)]² — acoustic impedance and intensity reflection coefficient at normal incidence.
  • I = I0·exp(−μ·x) and HVL = ln 2 / μ — radiation attenuation; μ = linear attenuation coefficient (m⁻¹), x = thickness (m).
  • Ug = F·t / D0 — radiographic geometric unsharpness; F = source size, t = object-to-film distance, D0 = source-to-object distance (mm).
  • δ = 1 / √(π·f·μ·σ) — eddy-current depth of penetration (m); μ = μ0·μr (μ0 = 4π × 10⁻⁷ H/m), σ = conductivity (S/m).

Corrosion and Its Prevention

  • m = I·t·M / (n·F) — Faraday's law; m = mass dissolved (g), I = current (A), t = time (s), M = molar mass (g/mol), n = electrons per atom, F = 96 485 C/mol.
  • CPR = 87.6·W / (ρ·A·t) — corrosion penetration rate (mm/year); W = mass loss (mg), ρ = density (g/cm³), A = area (cm²), t = time (h).
  • E°cell = E°cathode − E°anode — standard cell potential (V).