Patterns, Pattern Allowances and Core Making
L_p = L_c × (1 + α)— pattern dimension; L_c = casting dimension (mm) including machining allowance, α = linear shrinkage allowance (fraction). Applies to sizing patterns for solid contraction.Draft increase per side = h × tan θ— h = depth of the vertical face (mm), θ = draft angle.F_b = V_c × (ρ_m − ρ_c) × g— net upward force on a core (N); V_c = core volume in metal (m³), ρ_m, ρ_c = metal and core densities (kg/m³), g = 9.81 m/s². Applies to chaplet and core-print design.
Moulding Sands and Mould Making
PN = (V × H) / (p × A × t)— permeability number; V = air volume (cm³), H = specimen height (cm), p = pressure (g/cm² water), A = specimen area (cm²), t = time (min). For the standard specimen and 2000 cm³ of air,PN = 501.3 / (p × t).GFN = Σ(wᵢ × mᵢ) / Σwᵢ— grain fineness number; wᵢ = mass retained on sieve i, mᵢ = multiplier of that sieve.
Gating System Design and Pouring Time
v = √(2·g·h)— metal velocity at the sprue base or gate (m/s); h = metal head (m).Q = A·v— volume flow rate (m³/s) through the choke area A (m²).t_f = V / (A_g·√(2·g·h_t))— top-gating filling time (s); V = cavity volume (m³), A_g = gate area (m²), h_t = sprue height (m).t_f = (A_m / A_g) × (2/√(2g)) × (√h_t − √(h_t − h_m))— bottom-gating filling time (s); A_m = plan area of cavity (m²), h_m = cavity height (m).A_top / A_bottom = √(h_bottom / h_top)— sprue taper to avoid aspiration; h = metal head at each section.
Solidification, Chvorinov's Rule and Riser Design
t_s = B × (V/A)ⁿ— Chvorinov's rule; t_s = solidification time (s), B = mould constant (s/m² for n = 2, from experiment), V = volume (m³), A = cooling surface area (m²), n ≈ 2.t_riser / t_casting = (M_riser / M_casting)²— same mould, n = 2; M = V/A = modulus (m).M_riser ≥ 1.2 × M_casting— modulus criterion for a riser to freeze after the casting.
Special Casting: Die, Investment, Centrifugal, Shell
G = ω²·R / g— G-factor of a centrifugal mould; ω = angular speed (rad/s), R = mould inner radius (m).N = (60 / 2π) × √(G·g / R)— mould speed (rpm) for a chosen G-factor.p = ρ·ω²·(r_o² − r_i²) / 2— pressure of the rotating liquid on the mould wall (Pa); r_o, r_i = outer and inner radii of the metal layer (m).F_clamp ≥ p_inj × A_projected— die-casting clamp force (N); A_projected = cavities plus runners on the parting plane (m²).
Casting Defects and Inspection
d = v·t / 2— pulse-echo ultrasonic depth (m); v = sound velocity (m/s), t = round-trip time (s).V_r ≥ β·V_c / (η − β)— riser volume to feed shrinkage; β = solidification shrinkage (fraction), V_c = casting volume, η = riser efficiency (fraction of riser usable as feed).
Plastic Deformation, Yield Criteria and Hot vs Cold Working
ε = ln(L/L₀) = ln(h₀/h) = ln(A₀/A)— true strain (volume constant).σ_f = K·εⁿ— cold-working flow stress (MPa); K = strength coefficient (MPa), n = strain-hardening exponent.Ȳ = K·εⁿ / (1 + n)— average flow stress from 0 to ε (MPa).σ_f = C·ε̇ᵐ— hot-working flow stress (MPa); C = strength constant (MPa), ε̇ = strain rate (s⁻¹), m = strain-rate sensitivity.σ_max − σ_min = σ_y,k = σ_y / 2— Tresca criterion; k = shear yield stress.√(½[(σ₁ − σ₂)² + (σ₂ − σ₃)² + (σ₃ − σ₁)²]) = σ_y,k = σ_y / √3— von Mises criterion.Y′ = (2/√3)·σ_y ≈ 1.155·σ_y— plane-strain yield stress (von Mises).
Forging: Open-Die, Closed-Die and Forging Load
d₀²·h₀ = d²·h— volume constancy in upsetting a cylinder.F = p_avg × A— forging load (N); p_avg = average die pressure (Pa), A = current contact area (m²).p_avg ≈ σ_f × (1 + 2μr / (3h))— cylinder, Coulomb friction μ (small 2μr/h); r = radius, h = height.p_avg = σ_f × (1 + r / (3h))— cylinder, sticking friction.p_avg ≈ Y′ × (1 + μb / (2h))— plane-strain strip, Coulomb friction; b = strip width in flow direction, h = thickness.F = K_f × σ_f × A— empirical closed-die load; K_f = shape factor from data book, A = projected area including flash.
Rolling: Mechanics, Roll Force and Power
Δh = h₀ − h_f,Δh = 2R(1 − cos α)— draft (mm) and bite angle α; R = roll radius.L ≈ √(R·Δh)— projected contact length (mm).Δh_max = μ²·R— maximum draft for unaided bite;α_max = tan⁻¹ μ.h₀·w₀·v₀ = h_f·w_f·v_f— volume flow constancy; v = strip speed (m/s).F = Ȳ·w·L— roll force (N with Ȳ in MPa, w and L in mm); w = strip width.P = 2πN·F·L / 60— total power for both rolls (W, with L in m), taking the moment arm as 0.5L; N = roll speed (rpm).Forward slip = (v_f − v_r) / v_r— v_f = exit strip speed, v_r = roll surface speed.
Extrusion and Wire Drawing
R_x = A₀ / A_f— extrusion ratio;r = (A₀ − A_f) / A₀— reduction in area.p_ideal = Ȳ × ln(A₀/A_f)— ideal extrusion pressure (MPa).p = Ȳ × (a + b·ln R_x)— Johnson's empirical pressure; a ≈ 0.8, b ≈ 1.2–1.5 (use given values).F = p × A₀,P = F × v_ram— ram force (N) and power (W).σ_d = Ȳ × ((1 + B)/B) × [1 − (A_f/A₀)^B],B = μ·cot α— Sachs drawing stress; α = die half-angle.F_d = σ_d × A_f,P = F_d × v_f— drawing force (N) and power (W); v_f = exit speed.r_max = 1 − 1/e ≈ 0.632— ideal maximum reduction per drawing pass (perfectly plastic, frictionless).
Sheet Metal: Shearing, Blanking Force and Die Clearance
F = L × t × τ— blanking/punching force (N); L = cut perimeter (mm), t = thickness (mm), τ = shear strength (MPa).c = a × t— clearance per side (mm); a = clearance allowance (fraction).D_punch = D_blank − 2c(blanking, die = blank size);D_die = D_hole + 2c(punching, punch = hole size).W = F × p × t— work per stroke (J with t in m); p = fractional penetration at fracture.F_shear ≈ F × p × t / (p × t + s)— reduced peak force with shear s (mm) on punch or die (some texts use F·p·t / s).
Bending, Deep Drawing and Spinning
BA = α × (R + K·t)— bend allowance (mm); α = bend angle (rad), R = inner radius (mm), K = neutral-axis factor (0.33–0.5).e_outer = 1 / (1 + 2R/t)— engineering strain at the outer fibre.F_b = k_b × σ_UTS × w × t² / D— bending force (N); w = bend length (mm), D = die opening (mm), k_b ≈ 1.33 (V-bending), 0.33 (wiping).D = √(d² + 4·d·h)— blank diameter for a flangeless cylindrical cup (mm); d = cup diameter, h = height.DR = D / d_p ≤ LDR ≈ 2— drawing ratio and limit.F_d ≈ π × d_p × t × σ_UTS × (D/d_p − 0.7)— empirical maximum drawing force (N).t_f = t₀ × sin α— shear-spinning wall thickness; α = half-angle of the cone.
Powder Metallurgy: Powder Production, Compaction and Sintering
ρ = m / V,P = 1 − ρ / ρ_th— bulk density and porosity; ρ_th = pore-free density.1 / ρ_th = Σ wᵢ / ρᵢ— theoretical density of a mix from mass fractions wᵢ.F = p × A_p— press force (N); p = compaction pressure (Pa), A_p = projected area normal to the punch (m²).L_s / L_g = (ρ_g / ρ_s)^(1/3)— uniform sintering shrinkage from mass conservation; g = green, s = sintered.p_x = p₀ × exp(−4μkx / D)— pressure at depth x in single-action die compaction; μ = die-wall friction, k = radial/axial pressure ratio, D = die diameter.
Processing of Polymers, Ceramics and Composites
E_L = E_f·V_f + E_m·V_m— longitudinal modulus of an aligned continuous-fibre composite (iso-strain).1 / E_T = V_f / E_f + V_m / E_m— transverse modulus (iso-stress).ρ_c = ρ_f·V_f + ρ_m·V_m— composite density; V = volume fractions.F_clamp = p_c × A_p— injection-moulding clamp force (N); p_c = cavity pressure (Pa), A_p = projected area of all cavities and runners (m²).D_c = D_p / (1 − S)— mould cavity size; D_p = part size, S = linear shrinkage (fraction).Q_d = 0.5 × π² × D² × N × h × sin A × cos A— extruder drag flow (m³/s); D = screw diameter (m), N = speed (rev/s), h = channel depth (m), A = helix angle.
Arc Welding: SMAW, GMAW, GTAW and SAW
H = η × V × I / v— net heat input per unit length (J/mm); η = arc efficiency, V = arc voltage (V), I = current (A), v = travel speed (mm/s). With v in mm/min:H (kJ/mm) = η·V·I·60 / (1000·v).V_arc = A + B·l— linear arc characteristic; l = arc length (mm).V = OCV − (OCV / SCC) × I— drooping power-source line; OCV = open-circuit voltage, SCC = short-circuit current.P_max = OCV × SCC / 4atI = SCC / 2— maximum arc power for a linear source.m = ρ × (π d² / 4) × f— wire melting rate (kg/s); d = wire diameter (m), f = wire feed speed (m/s).
Heat Flow, Power Density and Weld Metallurgy
PD = P / A— power density (W/mm²); A = heated spot area.U_m = K × T_m²— unit melting energy (J/mm³); K = 3.33 × 10⁻⁶ J/(mm³·K²), T_m in kelvin.f₁ × f₂ × P = U_m × A_w × v— melting-energy balance; f₁ = heat-transfer factor, f₂ = melting factor, A_w = weld cross-section (mm²), v = travel speed (mm/s).R = 2π × k × (T_c − T₀)² / H_net— thick-plate centreline cooling rate (K/s); k = thermal conductivity (W/(mm·K)), T₀ = initial/preheat temperature, H_net in J/mm.CE = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15— IIW carbon equivalent (mass %).
Resistance, Gas and Solid-State Welding
H = I² × R × t— resistance-welding heat (J); I = current (A), R = effective resistance (Ω), t = time (s).η = U_m × V_n / H— fraction of heat used to melt the nugget of volume V_n (mm³).V_O₂ (cylinder) ≈ V_C₂H₂;V_O₂ (total) = 2.5 × V_C₂H₂— neutral oxy-acetylene flame and complete combustion.T = (2/3) × μ × p × π × R³,P = T × ω— friction-welding torque (N·m) for uniform pressure p on a bar of radius R, and power (W).
Brazing, Soldering and Adhesive Bonding
L = σ × t / τ— lap length for equal strength; σ = strip tensile strength, t = strip thickness, τ = filler/adhesive shear strength.τ × π × D × L = σ × (π/4) × (D² − d²)— insertion depth L of a tube (OD D, ID d) in a socket.F_max = τ × A_lap— lap-shear failure load (N).h = 2 × γ × cos θ / (ρ × g × c)— capillary rise between plates (m); γ = surface tension (N/m), θ = contact angle, c = gap (m).
Welding Defects and Inspection
d = v × t / 2— straight-beam UT depth; v = sound velocity (about 5.9 mm/µs in steel), t = round-trip time.depth = s × cos θ,surface distance = s × sin θ— angle-beam UT; s = sound path, θ = beam angle from the normal.U_g = F × d / D— radiographic geometric unsharpness (mm); F = focal-spot size, d = object-to-film distance, D = source-to-object distance.